為什么不銹鋼不能用碳鋼焊條焊接?

來源:http://niuniury.com/  發(fā)布時間:2022-03-29 瀏覽次數(shù):0

焊接是被焊工件的材質(zhì)(同種或異種),通過加熱或加壓或兩者并用,選擇是否使用填充材料,使工件的材質(zhì)達(dá)到原子間的結(jié)合,而形成長時間連接的工藝過程。那么不銹鋼焊接要點與注意事項有哪些呢?

Welding is a process in which the material of the workpiece to be welded (the same or different) is heated, pressurized or both, and whether the filler material is used is selected to make the material of the workpiece achieve the combination between atoms and form a long-time connection. So what are the key points and precautions of stainless steel welding?
1、焊不銹鋼用什么焊條或焊絲?
1. What kind of welding rod or wire is used to weld stainless steel?
不銹鋼焊條可分為鉻不銹鋼焊條和鉻鎳不銹鋼焊條,這兩類焊條中凡符合國標(biāo)的,均按國標(biāo)GB/T983-2012規(guī)定考核。
Stainless steel electrodes can be divided into chromium stainless steel electrodes and chromium nickel stainless steel electrodes. In these two types of electrodes, those that meet the national standard shall be assessed according to the provisions of the national standard GB / t983-2012.
鉻不銹鋼具有一定的耐蝕(氧化性酸、氣蝕)和耐熱性能,通常被選作電站、化工、石油等設(shè)備材料。但鉻不銹鋼一般情況下可焊性較差,應(yīng)注意焊接工藝、熱處理條件及選用合適的電焊條。鉻鎳不銹鋼焊條具有良好耐腐蝕性,廣泛應(yīng)用于化工、化肥、石油領(lǐng)域。為防止由于加熱而產(chǎn)生晶間腐蝕,焊接電流不宜太大,比碳鋼焊條小20%左右,電弧不宜過長,層間快冷,以窄焊道為宜。
Chromium stainless steel has certain corrosion resistance (oxidizing acid, cavitation) and heat resistance. It is usually selected as equipment materials for power station, chemical industry, petroleum and so on. However, the weldability of chromium stainless steel is generally poor. Attention should be paid to the welding process, heat treatment conditions and the selection of appropriate electrodes. Chromium nickel stainless steel electrode has good corrosion resistance and is widely used in the fields of chemical industry, chemical fertilizer and petroleum. In order to prevent intergranular corrosion due to heating, the welding current should not be too large, which is about 20% smaller than that of carbon steel electrode. The arc should not be too long and the interlayer should be cooled quickly. Narrow weld bead is appropriate.
2、不銹鋼焊接要點與注意事項
2. Key points and precautions for stainless steel welding
一、采用垂直外特性的電源,直流時采用正極性(焊絲接負(fù)極)
1、 The power supply with vertical external characteristics is adopted, and the positive polarity is adopted in DC (the welding wire is connected to the negative pole)
1、一般適合于6mm以下薄板的焊接,具有焊縫成形美觀,焊接變形量小的特點。
1. It is generally suitable for the welding of thin plates below 6mm, with the characteristics of beautiful weld formation and small welding deformation.
2、保護(hù)氣體為氬氣,純度為99.99%。當(dāng)焊接電流為50~150A時,氬氣流量為8~10L/min,當(dāng)電流為150~250A時,氬氣流量為12~15L/min。
2. The shielding gas is argon with a purity of 99.99%. When the argon flow is 150 ~ 15L / min, the argon flow is 150A ~ 15L / min.
3、鎢極從氣體噴嘴突出的長度,以4~5mm為佳。在角焊等遮蔽性差的地方是2~3mm,在開槽深的地方是5~6mm,噴嘴工作的距離一般不超過15mm。
3. The length of tungsten electrode protruding from the gas nozzle is preferably 4 ~ 5mm. It is 2 ~ 3mm in the place with poor shielding performance such as fillet welding, 5 ~ 6mm in the place with deep groove, and the distance from the nozzle to the working is generally no more than 15mm.
4、為防止焊接氣孔出現(xiàn),焊接部位如有鐵銹、油污等務(wù)必清理干凈。
4. In order to prevent the occurrence of welding pores, the welding parts must be cleaned if there is rust, oil stain, etc.
5、焊接普通鋼時,焊接電弧長度以2~4mm為佳;而焊接不銹鋼時,以1~3mm為佳,過長則保護(hù)效果不好。
5. When welding ordinary steel, the length of welding arc is 2 ~ 4mm; When welding stainless steel, it is better to use 1 ~ 3mm. If it is too long, the protection effect is not good.
6、對接打底時,為防止底層焊道的背面被氧化,背面也需要實施氣體保護(hù)。
6. During butt backing, in order to prevent the back of the underlying weld bead from being oxidized, the back also needs to be protected by gas.
7、為使氬氣很好地保護(hù)焊接熔池,和便于施焊操作,鎢極線與焊接處工件一般應(yīng)保持80°~85°角,填充焊絲與工件表面夾角應(yīng)盡可能小,一般為10°左右。
7. In order to protect the welding pool well with argon and facilitate the welding operation, the tungsten electrode line and the workpiece at the welding position shall generally maintain an angle of 80 ° ~ 85 °, and the included angle between the filler wire and the workpiece surface shall be as small as possible, generally about 10 °.
8、防風(fēng)與換氣。有風(fēng)的地方,務(wù)請采取擋網(wǎng)的措施,而在室內(nèi)則應(yīng)采取適當(dāng)?shù)膿Q氣措施。
8. Windproof and ventilation. Where there is wind, please take measures to block the net, and take appropriate ventilation measures indoors.

上一篇:等離子切割機(jī)穿孔后原地不走是什么原因?
下一篇:數(shù)控焊接操作時需要注意什么?

精品国产V无码大片在线观看 | 亚洲国产av无码精品无广告 | 蜜臀久久99精品久久久久久| 青青小草国产在线播放| 国产成人麻豆亚洲综合无码精品| 无码专区亚洲综合另类| 在线视频夫妻内射| 中文字幕精品一二三四五六七八 | 国产精品亚洲五月天高清| 男女猛烈无遮掩视频免费软件| 丝袜人妻一区二区三区| 人与动人物A级毛片在线| 国产福利自产拍| 色偷偷亚洲第一综合网| 久久婷婷五月综合色国产| 用舌头去添高潮无码视频| 亚洲2022国产成人精品无码区| 久久综合给合久久97色| 久久久久亚洲av成人片乱码| 国产精品99精品久久免费| 加勒比中文字幕无码一区| 欧美18-19sex性| 精品人妻无码视频中文字幕一区二区三区 | 亚洲AV永久无码精品天堂久久 | A级毛片免费观看完整| 欧美 国产 日产 韩国 在线| 国产美女视频国产视视频| 国产精品成人国产乱| 亚洲AV美女在线播放啊| 久久久久亚洲av成人网人人软件| 潮喷失禁大喷水aⅴ无码| 人妻熟妇乱又伦精品视频APP| 国产偷录视频叫床高潮| 97久久人人超碰国产精品| 成人性生交片无码免费看| 伊人亚洲综合影院首页| 国产va免费精品高清在线| 亚洲丶国产丶欧美一区二区三区| 99精品国产在热久久婷婷| 被三个男人绑着躁我好爽| 欧美mv国产mv日产mv|